MacDermid Alpha Micromax 5082R Silver Covering Conductor for LTCC Brazing

基础信息

品名
MacDermid Alpha Micromax 5082R Silver Covering Conductor
牌号
Micromax 5082R
厂商
Element Solutions/MacDermid Alpha
材料类型
Silver Conductor Paste / Low Temperature Braze System
产品形态
Paste
特点
High strength, high reliability attachment mechanism; hermetic packaging; compatibility with thick film resistors, as well as all conventional IC and lid attach processes; phthalate and cadmium free (no intentional addition)

描述




MacDermid Alpha Micromax 5082R Silver Covering Conductor for LTCC Brazing

Product: Micromax 5082R
Type: Silver Covering Conductor
Application: LTCC Ag/Pt Conductor
Series: 5081R + 5082R
Shelf Life: 6 months

⚡ Covering Silver Layer for Two-Component LTCC Brazing Systems
Micromax 5082R is the top silver covering conductor in a two-component thick film system with Micromax 5081R. It enables high temperature solders and low temperature braze alloys on 96% alumina and Micromax GreenTape 951 LTCC. Phthalate and cadmium free, with high strength attachment and hermetic packaging capability.

Micromax 5082R from MacDermid Alpha is the silver covering conductor in a two-component, all thick film system paired with Micromax 5081R. The system enables high temperature solders and low temperature braze alloys on 96% alumina and the Micromax GreenTape 951 low temperature cofired ceramic system. It is also compatible with thick film resistors and conventional IC and lid attach processes. The formulation is phthalate and cadmium free.

The paste has a viscosity range of 225–325 Pa.s and uses Micromax 9180R as the recommended thinner. Print 5082R over the fired 5081R using a 325-mesh stainless steel screen with 13μm emulsion, at room temperature 20–23°C. Ensure 5082R completely covers the 5081R print. Allow prints to level over 10 minutes, then dry 10–15 minutes at 150°C. Fire at 850°C peak held for 10 minutes on a 30-minute cycle in air atmosphere. Total 5082R fired thickness should exceed 20 μm; the exact thickness depends on the braze alloy and brazing temperature. PGA reliability is ≥15 lbs under both thermal cycle (−40°C to 125°C, 200 cycles) and thermal aging (200 hrs in air at 150°C). Seal ring reliability is below 10⁻⁸ Atm cm³/s by helium leak test. Brazing is performed in nitrogen atmosphere with Au/Sn alloys, preforms, or pastes. Store sealed at 5–30°C; unopened shelf life is 6 months.

Genuine MacDermid Alpha Micromax Imported Stock & Technical Support
We hold regular stock of authentic MacDermid Alpha Micromax 5082R silver covering conductor paste. Original factory TDS and batch-specific COA are available on request for your LTCC and brazing programs.

Request Sample, TDS & Quotation
Complete TDS, COA, and regulatory documentation available

Key Features of MacDermid Alpha Micromax 5082R

  • Silver covering conductor paste for the two-component 5081R / 5082R thick film system
  • Printed over the fired 5081R and must fully cover it
  • Phthalate and cadmium free formulation (no intentional addition)
  • High strength, high reliability attachment mechanism
  • Supports hermetic packaging with seal ring reliability <10⁻⁸ Atm cm³/s
  • Enables high temperature solders and low temperature braze alloys
  • Compatible with thick film resistors and conventional IC and lid attach processes
  • Suited to 96% alumina and Micromax GreenTape 951 LTCC substrates
  • Viscosity 225–325 Pa.s for stable screen printing
  • Screen: 325-mesh stainless steel with 13μm emulsion
  • Firing: 850°C peak held 10 minutes on 30-minute cycle in air
  • Total 5082R fired thickness >20 μm; PGA reliability ≥15 lbs under thermal cycle and thermal aging

Primary Applications

  • LTCC Ag/Pt conductors — covering silver layer on GreenTape 951 and 96% alumina
  • Multilayer hybrid circuits — top conductor layer in complex hybrid builds
  • Hermetic brazed assemblies — pin, window frame, and heat sink attachment
  • IC and lid attach — compatible with conventional IC and lid attach processes

Full Technical Specifications

Property Typical Value TDS Reference
Product Type Silver covering conductor paste TDS: Silver Brazing Low Temperature Braze System
Application LTCC Ag/Pt conductor TDS: LTCC Ag/Pt conductor
Solvent or Thinner Micromax 9180R TDS: Micromax 9180R
Blend Member or Series 5081R and 5082R TDS: 5081R and 5082R
Viscosity 225 to 325 Pa.s TDS: Brookfield 2xHA, SC4-14/6R, 10 rpm, 25°C
Screen Type 325-mesh stainless steel with 13 μm emulsion TDS: 325-mesh, 13μm emulsion
Printing Requirement Printed over fired 5081R; must completely cover the 5081R print TDS: ensure 5082R completely covers the 5081R print
Printing Room Temperature 20 to 23 °C TDS: 20°C - 23°C
Printing Area Class 10,000 recommended for complex hybrids and multilayer circuits TDS: Class 10,000 printing area
Leveling Over 10 minutes at room temperature TDS: over 10 minutes
Drying Schedule ≥10–15 minutes at 150°C TDS: ≥10-15 minutes at 150°C
Firing Profile 850°C peak held 10 minutes on 30-minute cycle, air atmosphere TDS: 850°C peak, 10 min hold, 30 min cycle
Total 5082R Fired Thickness > 20 μm TDS: >20μm
PGA Reliability Thermal Cycle ≥ 15 lbs (200 cycles, −40°C to 125°C rapid transfer) TDS: ≥15 lbs
PGA Reliability Thermal Aging ≥ 15 lbs (200 hrs in air at 150°C) TDS: ≥15 lbs
Seal Ring Reliability < 10⁻⁸ Atm cm³/s (He leak, 100 thermal cycles −25°C to +85°C) TDS: <10⁻⁸
Phthalate and Cadmium Free Yes (no intentional addition) TDS: Product benefits
Brazing Atmosphere Nitrogen TDS: nitrogen atmosphere
Brazing Alloys Au/Sn braze alloys, preforms, or pastes TDS: Au/Sn, preforms or pastes
Shelf Life 6 months TDS: 6 months
Storage Temperature 5 - 30 °C TDS: 5°C - 30°C

Note: All listed values are typical and may vary by batch. Values based on MacDermid Alpha official TDS. Independent qualification testing is required prior to production use. "Phthalate and cadmium free" as used herein means these substances are not intentional ingredients and are not intentionally added. Trace amounts may be present.

Recommended Processing Conditions

Parameter Recommended Value TDS Reference
Mixing Prior to Use Slow, gentle hand stirring 1–2 minutes with clean burr-free spatula; avoid air entrapment TDS: 1-2 minutes
Room Temperature Before Printing 20 to 23 °C TDS: 20°C - 23°C
Screen Mesh 325-mesh stainless steel with 13 μm emulsion TDS: 325-mesh, 13μm
Printing Sequence Print 5082R over the fired 5081R; ensure 5082R completely covers 5081R TDS: Print onto fired 5081R
Leveling Over 10 minutes at room temperature TDS: over 10 minutes
Drying ≥10–15 minutes at 150°C in well-ventilated oven or conveyor dryer TDS: ≥10-15 min at 150°C
Firing 850°C peak held 10 minutes on 30-minute cycle, air atmosphere TDS: 850°C peak, 30 min cycle
Fired Thickness Total 5082R fired thickness >20 μm, depending on braze alloy and brazing temperature TDS: >20μm
Thinning Not normally required; Micromax 9180R for minor adjustment TDS: Micromax 9180R
Brazing Nitrogen atmosphere with Au/Sn braze alloys, preforms, or pastes TDS: nitrogen atmosphere

Handling and Storage Recommendations

Storage Rules Store tightly sealed in a clean, stable environment at 5-30°C. TDS: 5°C - 30°C
Shelf Life 6 months in unopened containers from date of shipment. TDS: 6 months
Pre-use Preparation Thoroughly mix prior to use. Some settling of solids may occur during storage. TDS: thoroughly mix
Contamination Control Keep paste, screens, and tools free of metal contamination. Dust and lint can contribute to poor yields. TDS: free of metal contamination
Transportation Under normal shipping conditions, no temperature control is expected. For extended transport periods, confirm product suitability. TDS: normal shipping conditions

Official Technical Documentation

Document Type Document Introduction Document Request
TDS MacDermid Alpha Micromax 5082R original factory technical data sheet Request TDS
COA Batch-specific certificate of analysis Request COA
SDS Safety Data Sheet for handling and storage Request SDS

Frequently Asked Questions

Why is 5082R used together with 5081R?

The TDS describes 5081R and 5082R as a two-component, all thick film paste system. 5081R is printed first onto the fired substrate; 5082R is printed afterward as the covering conductor. Together they enable high temperature solders and low temperature braze alloys.

How much 5082R thickness is required after firing?

Total 5082R fired thickness should exceed 20μm. The exact thickness depends on the type of braze alloy and the brazing temperature used.

Which substrates suit the 5081R / 5082R system?

Two substrate families are named in the TDS: 96% alumina and Micromax GreenTape 951 LTCC. Multilayer hybrid circuits are also covered under the application scope.

How strong is the brazed joint after thermal cycling?

PGA reliability is ≥15 lbs after 200 cycles from −40°C to 125°C rapid transfer. PGA reliability after thermal aging is also ≥15 lbs after 200 hours in air at 150°C.

How does 5082R perform in hermetic seal testing?

Seal ring reliability is below 10⁻⁸ Atm cm³/s by helium leak test on a Kovar seal ring bonded to Micromax 951 GreenTape, across 100 thermal cycles from −25°C to +85°C.

Is 5082R free of phthalate and cadmium?

Per the TDS, phthalate and cadmium oxide are not intentional ingredients and are not intentionally added. Trace amounts may be present. Customers with strict compliance thresholds should verify against their own requirements.

What thinner should be used with 5082R?

Micromax 9180R is the listed solvent or thinner. Thinning is not normally required since the composition is optimized for screen printing. Use it only for small viscosity adjustments or to replace evaporation loss.

Get MacDermid Alpha Micromax 5082R Bulk Pricing and Technical Support

We supply authentic MacDermid Alpha Micromax 5082R silver covering conductor paste for LTCC and brazing programs. Contact our team for bulk quotations, sample availability, technical documentation, and application support.

Inquire Bulk Price & Technical Support

Disclaimer: All technical data on this page are for general guidance only and are not product specifications. Buyers must carry out independent trials and verify suitability before bulk ordering. Actual values may vary between production lots. "Phthalate and cadmium free" as used herein means these substances are not intentional ingredients and are not intentionally added. Trace amounts may be present.

Technical Documents

Download technical data sheets, safety data sheets and certificates for this material.

TDS Files

Technical document available for review or download.

1 Files

MSDS Files

Technical document available for review or download.

0 Files
No MSDS file uploaded yet.