Santoprene 8201-50W185 TPV | ASTM F477 Pipe Seal TPV

基础信息

品名
Santoprene 8201-50W185
牌号
8201-50W185
厂商
Celanese Corporation
材料类型
Thermoplastic Vulcanizate (TPV) / Thermoplastic Elastomer (TPE)
产品形态
Pellets
特点
53 Shore A natural TPV, pipe-seal grade, improved compression-set performance, non-hygroscopic, colorable, ASTM F477 Low Head performance, good chemical resistance, shear-dependent flow, injection molding and extrusion processability, polyolefin-based construction and manufacturing-stream recyclability

描述

Santoprene 8201-50W185 is a soft, natural and colorable thermoplastic vulcanizate from Celanese developed specifically for pipe sealing applications requiring improved compression-set performance.

A major distinction of this grade is its positioning for ASTM F477 Low Head pipe seals.

The material combines rubber-like sealing behavior with the manufacturing advantages of a thermoplastic, allowing it to be processed on conventional injection-molding and extrusion equipment.

Current grade-specific Celanese Materials Database values include:

  • 52.7 Shore A hardness
  • 0.890 g/cm³ density
  • 498% elongation at break
  • 5.3 MPa tensile stress at break
  • 1.51 MPa stress at 100% elongation
  • 22% compression set at 23°C / 168 h

Celanese’s Product Finder and ASTM F477 application documentation use another qualification data set, showing approximately:

  • 53 Shore A
  • 575% elongation
  • 5.1 MPa tensile strength
  • 1.5 MPa 100% modulus
  • 22% compression set at 70°C / 22 h

These figures should not be treated as contradictory. They come from different published test programs and methods.

For SEO and commercial use, the most important positioning of Santoprene 8201-50W185 is:

ASTM F477 pipe seal TPV + improved compression set + non-hygroscopic + natural/colorable + 53 Shore A.

For more TPV products, visit our TPV Thermoplastic Vulcanizates Product Category →.

For current Santoprene portfolio information, see the Official Celanese Santoprene & Geolast Product Finder →.

Key Features of Santoprene 8201-50W185

Feature Engineering Benefit
Approx. 53 Shore A Hardness Provides a soft elastomeric response for pipe sealing
Natural / Colorable Allows customized color formulations
ASTM F477 Low Head Specifically developed for low-head pipe seal requirements
Improved Compression Set Supports long-term sealing recovery
Non-Hygroscopic Simplifies moisture handling in normal production
498% ISO Elongation Provides substantial flexibility and deformation capability
5.3 MPa ISO Tensile Stress at Break Provides useful mechanical strength
1.51 MPa Stress at 100% Elongation Supports flexible gasket behavior
Low Density Approx. 0.890 g/cm³
Good Chemical Resistance Useful in pipe, water and drainage environments
Injection Moldable Suitable for molded sealing rings and gaskets
Extrudable Suitable for continuous flexible sealing profiles
Shear-Dependent Flow Apparent viscosity decreases at higher shear rates
Polyolefin-Based TPV Combines elastomeric properties with thermoplastic processing
Manufacturing-Stream Recyclability Controlled clean process scrap can be reprocessed

Typical Applications for Santoprene 8201-50W185

Santoprene 8201-50W185 is particularly suitable for pipe and construction sealing systems.

Application Area Typical Use
Drainage Pipe Seals Flexible seals for drainage pipe joints
Sewer Pipe Gaskets Compression sealing around pipe connections
Low-Head Pipe Seals Applications designed around ASTM F477 requirements
Pipe Joint Gaskets Flexible interfaces between pipe sections
Push-Fit Pipe Seals Elastomeric sealing rings
Building Drainage Systems Flexible sealing components
Construction Seals Molded or extruded elastomer components
Water-System Seals Selected non-pressure sealing applications
Flexible Gaskets Injection-molded compression seals
Extruded Sealing Profiles Continuous TPV sealing sections

The strongest application keyword for this particular grade is pipe seal, rather than simply describing it as a general-purpose TPV.

Typical Properties of Santoprene 8201-50W185

Physical Properties

Property Typical Value Test Method
Density 890 kg/m³ / 0.890 g/cm³ ISO 1183
Shore A Hardness, 15 s 52.7 ISO 48-4 / ISO 868
Commercial Hardness Reference 53 Shore A Celanese Product Finder
Appearance Natural / Colorable Manufacturer Information
Product Form Pellets Manufacturer Information
Resin Identification TPV ISO 1043
Part Marking Code >TPV< ISO 11469

The grade name contains 50, but the current published typical hardness is approximately 52.7–53 Shore A.

Mechanical Properties

Current ISO Grade Data

Property Typical Value Test Method
Tensile Stress at 100% Elongation 1.51 MPa ISO 37
Tensile Stress at Break 5.3 MPa ISO 527-1/-2 / ISO 37
Elongation at Break 498% ISO 527-1/-2 / ISO 37
Compression Set, 23°C / 168 h 22% ISO 815
Shore A Hardness 52.7 ISO 48-4 / ISO 868

These are the current grade-specific Celanese Materials Database values and should be used as the main technical table for the product page.

ASTM F477 Low Head Pipe Seal Performance

One of the most important reasons to select Santoprene 8201-50W185 is its documented positioning against ASTM F477 Low Head pipe-seal requirements.

Celanese published the following application-level values:

Property ASTM F477 Requirement Santoprene 8201-50W185
Shore A Hardness 40–70 53
Tensile Strength ≥3.0 MPa 5.1 MPa
100% Modulus ≥1.4 MPa 1.5 MPa
Elongation at Break ≥350% 575%
Compression Set, 70°C / 22 h ≤25% 22%
Low-Temperature Hardness Increase at -10°C ≤10 points 5 points
Water Absorption / Volume Increase, 70°C / 48 h ≤4% 0.4%
Force Decay / Remaining Stress ≥40% 47.4%

This ASTM application data is especially valuable for customers manufacturing:

  • Pipe seals
  • Drainage gaskets
  • Sewer pipe joints
  • Low-head sealing rings
  • Infrastructure pipe components

Improved Compression-Set Performance

Compression set is critical in pipe seals because the gasket may remain compressed inside a joint for an extended period.

A sealing material should maintain enough recovery to continue applying pressure against the pipe interface.

For Santoprene 8201-50W185, Celanese specifically highlights improved compression set.

Published values include:

  • 22% at 23°C / 168 h in current ISO grade data
  • 22% at 70°C / 22 h in the ASTM F477 application test program

This makes compression-set performance one of the strongest technical selling points for the grade.

Potential applications include:

  • Pipe socket seals
  • Push-fit sealing rings
  • Drainage joints
  • Compression gaskets
  • Long-term static seals

Low-Temperature Pipe Seal Performance

ASTM F477 qualification data also includes low-temperature hardness behavior.

At -10°C, Santoprene 8201-50W185 showed an approximately 5 Shore A point hardness increase in the published Celanese application test.

This is below the listed ASTM F477 maximum of 10 points.

For pipe sealing, controlled low-temperature hardness change is important because an elastomer that becomes excessively stiff may:

  • Become harder to install
  • Provide less conformity to mating surfaces
  • Increase insertion force
  • Lose sealing flexibility

Water Absorption Performance

Pipe seals may remain in contact with water for extended periods.

In Celanese’s ASTM F477 application testing, Santoprene 8201-50W185 showed approximately:

0.4% volume increase after 48 hours at 70°C in water

against a listed maximum requirement of 4%.

Low water uptake helps support:

  • Dimensional stability
  • Seal geometry
  • Consistent compression
  • Long-term pipe-joint performance

Force Decay / Stress Retention

A pipe gasket is continuously compressed after installation.

For this reason, long-term force retention can be just as important as initial hardness.

Published ASTM F477 application testing showed approximately:

47.4% remaining stress

against a minimum listed requirement of 40%.

This property helps support long-term sealing pressure within the pipe joint.

Natural & Colorable Formulation

Santoprene 8201-50W185 is supplied in a Natural formulation.

This makes it suitable for applications requiring:

  • Gray seals
  • White components
  • Blue pipe-system identification
  • Colored drainage seals
  • Customized customer colors

Compatible masterbatch should be selected to maintain:

  • Mechanical properties
  • Compression-set performance
  • Surface quality
  • Processing stability

For regulated pipe applications, final color concentrate compatibility should also be considered during qualification.

Non-Hygroscopic Behavior

Another important characteristic of Santoprene 8201-50W185 is its non-hygroscopic formulation.

The material does not absorb atmospheric moisture in the same way as strongly hygroscopic engineering polymers.

This provides practical benefits including:

  • Easier material handling
  • Reduced drying sensitivity
  • More stable storage
  • Simpler production preparation

However, the current Celanese grade-specific processing sheet still recommends controlled drying before injection processing.

Therefore, “non-hygroscopic” should not be interpreted as meaning drying can never be useful.

Why Choose Santoprene 8201-50W185?

The strongest reason to select Santoprene 8201-50W185 is its specialized balance of sealing properties and pipe-application performance.

The grade provides:

  • Approx. 53 Shore A hardness
  • 0.890 g/cm³ density
  • 498% ISO elongation
  • 5.3 MPa ISO tensile stress at break
  • 1.51 MPa stress at 100% elongation
  • 22% compression set
  • Natural/colorable appearance
  • Non-hygroscopic formulation
  • Improved compression-set performance
  • ASTM F477 Low Head pipe-seal positioning
  • Good water-exposure performance
  • Good low-temperature hardness retention
  • Injection and extrusion processing
  • Shear-dependent flow

For customers manufacturing pipe gaskets, drainage seals, sewer seals and low-head sealing components, Santoprene 8201-50W185 is a highly relevant TPV grade.

Processing Guidelines for Santoprene 8201-50W185

Current grade-specific Celanese processing information lists:

  • Injection Moulding
  • Extrusion

The grade is shear dependent and can be processed using conventional thermoplastic equipment.

Drying Conditions

Processing Parameter Celanese Guidance
Drying Recommended Yes
Drying Temperature 80°C
Drying Time ≥3 hours
Dryer Type Dehumidified / Desiccant Dryer
Maximum Processing Moisture ≤0.08%
Maximum Regrind Level 20%

Despite the material being described as non-hygroscopic, these current grade-specific conditions should be used for controlled processing.

Injection Molding Conditions

Processing Parameter Celanese Guidance
Optimum Melt Temperature 200°C
Minimum Melt Temperature 185°C
Maximum Melt Temperature 220°C
Optimum Mold Temperature 30°C
Minimum Mold Temperature 10°C
Maximum Mold Temperature 50°C
Screw Speed 100–200 rpm
Holding Pressure 50–75% of actual injection pressure
Back Pressure 0.3–0.7 MPa when required

These are 8201-50W185-specific settings, so they are more useful than applying a generic Santoprene processing window.

Optimum Melt Temperature

The recommended initial melt-temperature target is:

200°C

with a grade-specific window of approximately:

185–220°C

This allows the processor to optimize:

  • Filling
  • Surface appearance
  • Cycle time
  • Part dimensions
  • Seal quality

Mold Temperature

The recommended mold-temperature range is:

10–50°C

with approximately:

30°C optimum

The actual mold setting depends on:

  • Seal thickness
  • Mold design
  • Gate position
  • Cycle-time target
  • Surface requirements
  • Part-release behavior

Screw Speed

Celanese recommends a relatively high screw speed:

100–200 rpm

Santoprene TPV is shear dependent, so increased shear can significantly reduce apparent melt viscosity.

This supports efficient filling without relying entirely on higher temperature.

Holding Pressure

Recommended holding pressure is approximately:

50–75% of the actual injection pressure

Holding pressure should be optimized to control:

  • Part dimensions
  • Sink
  • Packing
  • Seal geometry
  • Surface quality

Excessive packing is generally unnecessary for flexible TPV parts.

Back Pressure

Back pressure is not always required.

Where improved melt homogeneity is needed, Celanese recommends approximately:

0.3–0.7 MPa

Higher back pressure can also be helpful when using color masterbatch.

Shear-Dependent Flow

Santoprene 8201-50W185 is shear dependent.

As shear rate increases:

apparent melt viscosity decreases.

This makes factors such as:

  • Screw speed
  • Injection speed
  • Gate dimensions
  • Extrusion die design

important when developing the process.

Increasing temperature alone is not always the most effective way to improve TPV flow.

Extrusion Processing

Santoprene 8201-50W185 can also be processed by extrusion.

This makes it relevant to continuous sealing profiles and pipe-gasket geometries.

Important extrusion variables include:

  • Barrel temperatures
  • Screw design
  • Melt temperature
  • Melt pressure
  • Die geometry
  • Line speed
  • Cooling
  • Profile calibration

For pipe seals, dimensional control is especially important because gasket cross-section directly affects installation and sealing pressure.

Pipe-Seal Design Considerations

When using Santoprene 8201-50W185 for a pipe seal, engineers should consider:

  • Groove dimensions
  • Seal cross-section
  • Compression ratio
  • Insertion force
  • Pipe tolerance
  • Joint movement
  • Long-term force decay
  • Water exposure
  • Temperature range
  • Installation conditions

ASTM F477 material performance is an important starting point, but final pipe-joint performance also depends on component geometry.

Heat Aging

Celanese’s ASTM F477 application testing also evaluated heat aging at 70°C for 96 hours.

Published changes included approximately:

  • -1 Shore A point hardness change
  • 2.6% loss in tensile strength
  • 12% loss in elongation

These results support the grade’s pipe-seal positioning under the specified test conditions.

They should not be interpreted as a universal service-life prediction.

Material Compatibility

Santoprene TPV should be processed with appropriate purge procedures.

Particular care should be taken when transitioning from:

  • POM / Acetal
  • PVC

Contamination can affect:

  • Processing stability
  • Surface quality
  • Mechanical properties
  • Finished seal consistency

Manufacturing-Stream Recyclability

Santoprene 8201-50W185 is polyolefin based and can be recycled within appropriate manufacturing streams.

Clean controlled process scrap may include:

  • Sprues
  • Runners
  • Start-up material
  • Profile trim
  • Selected rejected parts

The current Celanese grade sheet permits up to approximately 20% regrind as a processing reference.

For qualified ASTM F477 products, the manufacturer should ensure that any regrind use remains compatible with the final product’s required performance.

Related Products

We supply Santoprene TPV grades for different pipe-sealing, construction, hardness and processing requirements.

Typical product families include:

  • Santoprene 8201 Series
  • Santoprene pipe-seal TPV grades
  • Santoprene ASTM F477 grades
  • Santoprene low-compression-set grades
  • Santoprene natural/colorable TPV
  • Santoprene injection-molding grades
  • Santoprene extrusion grades
  • Santoprene building and construction grades
  • Santoprene gasket materials

View More TPV Thermoplastic Vulcanizates →

Technical Documents for Santoprene 8201-50W185

Document Type Description
TDS Physical, mechanical and processing data
SDS Safety Data Sheet
ASTM F477 Information Low Head pipe-seal performance information
Pipe Seal Application Data Water absorption, force decay and low-temperature data
Injection Molding Guide Grade-specific molding recommendations
Extrusion Information Pipe-seal and profile processing guidance
COA Batch-specific quality documentation where available

Need technical documents for Santoprene 8201-50W185?

📧 Email: ruiqingchem@gmail.com

📝 Online form: Contact Us →

Please state Santoprene 8201-50W185 and specify whether you require TDS, SDS, ASTM F477 information, processing guidance or COA.

FAQ About Santoprene 8201-50W185

Q1: What is Santoprene 8201-50W185?

Santoprene 8201-50W185 is a natural, colorable TPV from Celanese specifically designed for pipe-seal applications and ASTM F477 Low Head requirements.

Q2: What is the hardness of Santoprene 8201-50W185?

Current data is approximately 52.7–53 Shore A.

Q3: Is the “50” in 8201-50W185 the exact hardness?

No. The grade designation contains 50, while current published typical hardness is approximately 53 Shore A.

Q4: What is the density?

Current grade-specific ISO data gives approximately 0.890 g/cm³.

Q5: What is the tensile stress at break?

Current ISO grade data gives approximately 5.3 MPa.

Q6: What is the elongation at break?

Current ISO grade data gives approximately 498%. Celanese’s separate ASTM F477 application test reports approximately 575%, so the test basis should be stated when using either number.

Q7: What is the stress at 100% elongation?

The current ISO grade-specific value is approximately 1.51 MPa.

Q8: What is the compression set?

Current grade data gives approximately 22% at 23°C / 168 h. Celanese’s ASTM F477 application testing also reports 22% at 70°C / 22 h.

Q9: Does Santoprene 8201-50W185 meet ASTM F477?

Yes. Celanese specifically positions Santoprene 8201-50W185 as meeting ASTM F477 Low Head requirements for pipe-seal applications.

Q10: Is Santoprene 8201-50W185 suitable for drainage pipe seals?

Yes. Pipe seals and drainage sealing are among the primary applications for this grade.

Q11: Is Santoprene 8201-50W185 non-hygroscopic?

Yes. Celanese describes it as non-hygroscopic.

Q12: Can Santoprene 8201-50W185 be colored?

Yes. The standard material is Natural / colorable.

Q13: Can Santoprene 8201-50W185 be injection molded?

Yes. Injection molding is a listed processing method.

Q14: Can Santoprene 8201-50W185 be extruded?

Yes. Extrusion is also listed for the grade.

Q15: What melt temperature is recommended?

Current grade-specific guidance gives approximately 185–220°C, with 200°C optimum.

Q16: What mold temperature is recommended?

The current recommended range is approximately 10–50°C, with 30°C optimum.

Request Santoprene 8201-50W185 Price & Technical Support

For pricing, availability, technical documentation or application support for Santoprene 8201-50W185, please provide:

  • Required quantity
  • Destination country or port
  • Pipe / drainage / sewer application
  • Pipe diameter
  • Seal geometry
  • ASTM F477 requirement
  • Low Head requirement
  • Required hardness
  • Compression-set requirement
  • Water-contact conditions
  • Operating temperature
  • Injection or extrusion process
  • Required color
  • TDS / SDS requirement
  • ASTM F477 documentation requirement
  • COA requirement
  • Sample requirement, if applicable

📧 Email: ruiqingchem@gmail.com

📝 Send Inquiry →

Technical Documents

Download technical data sheets, safety data sheets and certificates for this material.

TDS Files

Technical document available for review or download.

0 Files
No TDS file uploaded yet.

MSDS Files

Technical document available for review or download.

0 Files
No MSDS file uploaded yet.